How do I fix weld undercut?

Fill the groove and correct the cause

JOPLIN, Missouri — Weld undercut is a groove melted into the base metal along the edge of a weld and left unfilled. Fix it by cleaning the area, filling the groove with a small stringer bead using lower heat, then correcting the settings or technique that caused it. Undercut matters because it thins the metal and creates a notch where cracks start, especially on parts that flex or carry load.

Spot the problem

Look along the toe of the weld, the edge where the bead meets the base metal. Undercut shows as a groove or notch. Run a fingernail or a thin pick along the edge, and use good light. Minor, shallow undercut on a non-critical weld might be acceptable, but deeper grooves on structural, fatigue-loaded or pressure parts should be repaired. Codes set limits for critical work, so ask a certified inspector if the part is important.

Why it happens

The most common causes are too much amperage or voltage, which melts the edge faster than filler can fill it; travel speed too fast; a wrong electrode angle that points the arc at one side; too long an arc; and pausing wrong when weaving. In vertical and overhead welding, gravity pulls the puddle away from the edge. Wrong gas mix on MIG and an overly large electrode can also play a part.

Prepare the repair

Clean the weld and groove of slag, spatter and contamination with a wire brush or light grinding. Don't grind so deeply that you thin the part further. If the groove is deep or sharp, blend the edge slightly so the filler can fuse into it. Make sure the metal is dry and clean.

Fill the groove

Use a small-diameter electrode or wire and reduced current. Run a narrow stringer bead along the undercut, directing the arc into the groove and slightly onto the base metal, so the filler wets in at both sides. For stick, keep a short arc and a steady speed; for MIG, keep a short stickout and a steady travel. Check that the new bead blends smoothly into the base metal without creating a new groove. Several light passes beat one hot pass.

Correct the cause

Turn down the heat a notch and test on scrap. Adjust the angle so the arc favors the thicker or lower piece. When weaving, pause briefly at each edge so the puddle fills the toe, then move across quickly. Keep the arc short and the speed steady. If you're welding in position, use smaller electrodes and lower amperage, and consider a weave pattern suited to the position.

Check the result

After repair, inspect the weld toes in good light, and use dye penetrant on critical parts. A smooth, gradual transition from weld to base metal is the goal. Test a sample weld on scrap with the same settings before you go back to the real part.

Know when to ask for help

For lifting equipment, trailers, hitches or pressure components, have a certified welder or inspector review any undercut repair. For shop safety, see the OSHA agriculture page and the CDC NIOSH agriculture program. Learning resources are at extension.org and extension.purdue.edu. Fixing undercut is a small job, and keeping it from happening is mostly a matter of slowing the arc down and aiming it where the metal needs it.